Trimmer Posted February 18, 2012 Posted February 18, 2012 I just put a coat of kast-o-lite in my forge. When can I coat it with the plistix? Do I wait until the kast-o-lete is dry, or put the plistix in and let it all dry together? Thanks for the help, Trimmer Quote
WayneCoeArtistBlacksmith Posted February 18, 2012 Posted February 18, 2012 I suggest that you wait until the Kast-0-Lite has cured. After casting is set (the next day) I put the forge in the oven (I have an oven in my shop and don't have to get permission) at 500 degrees F for about 4 hours. This will speed up the curing. I then paint on the Plistix after the forge is back to room temprature. Then wait for it to dry before firing the forge. Quote