I was finally successful in creating a hamon!
W2 file normalized, annealed, shaped, then my attempt at hamon clay, light oil quench, and 390 degree temper.
post-25471-0-87903900-1353209606_thumb.j
post-25471-0-43246300-1353209614_thumb.j
The process was first all tested with pieces of an similar file. I found water quench yielded cracks, so I went over to oil. Here's a few pics of testing, drying clay, and post tests next to right outta the oil.
post-25471-0-43642800-1353210002_thumb.j
post-25471-0-56934600-1353209966_thumb.j
post-25471-0-76882000-1353209925_thumb.j
Since it's to be used in a kitchen I went ahead and gave it an acid bath; plus I just like the way it makes the hamon pop.
What do you guys think?

Link to comment
Share on other sites

Good start and interesting effect.

Ive been bitten by the hamon bug as well and have been doing a ton of research on the stuff. One thing I would suggest is raise the thick portion of the clay a little higher and thin it out some. Probably only needs to be around 1/8" thick, also thin out some and do a little transition area of thinner stuff. Worth a shot. Im still playing with it all as well. They are fun, never quiet know what your gonna get.

Link to comment
Share on other sites

Join the conversation

You can post now and register later. If you have an account, sign in now to post with your account.

Guest
Reply to this topic...

×   Pasted as rich text.   Paste as plain text instead

  Only 75 emoji are allowed.

×   Your link has been automatically embedded.   Display as a link instead

×   Your previous content has been restored.   Clear editor

×   You cannot paste images directly. Upload or insert images from URL.

×
×
  • Create New...